A spacecraft power supply intended for operation in the intense radiation environment near Jupiter was able to continue functioning after a detailed failure analysis of its switching stage. The unit converts a nominal 28 V input into +5 V, +3.3 V, and -5 V rails for onboard sensors, and its primary power conversion stage uses two IRHNJ57024 N-channel MOSFET1. metal-oxide semiconductor field effect transistorVoltage-controlled field-effect transistor with an insulated gate, widely used in integrated circuits.2. metal-oxide-semiconductor field-effect transistorA common transistor type used here as the layout and technology reference.s driven through a gate-drive transformer.
The circuit architecture combines galvanic isolation between the PWMpulse width modulationPulse width modulation controls an output quantity by varying the duty cycle of a periodic control signal. controller and the switching stage with separate power and control grounds. That isolation is meant to protect the low-voltage control circuitry from failures, voltage spikes, and switching noise generated in the power stage. The design also recovers energy from transformer leakage inductance during MOSFET1. metal-oxide semiconductor field effect transistorVoltage-controlled field-effect transistor with an insulated gate, widely used in integrated circuits.2. metal-oxide-semiconductor field-effect transistorA common transistor type used here as the layout and technology reference. turn-off and returns it to the DCdirect currentElectric current that flows in one direction.-link capacitors, improving converter efficiency.
High-amplitude spikes and transient noise produced by the MOSFET1. metal-oxide semiconductor field effect transistorVoltage-controlled field-effect transistor with an insulated gate, widely used in integrated circuits.2. metal-oxide-semiconductor field-effect transistorA common transistor type used here as the layout and technology reference. switching action were reduced with snubbers that had been tuned using measurements. The PWMpulse width modulationPulse width modulation controls an output quantity by varying the duty cycle of a periodic control signal. controller uses voltage feedback and current sensing to regulate the outputs and enforce current limiting, while the RAMPReliability Analysis and Modeling Program_NIM2 signal provides a current-related feedback path to the controller.
After launch, further testing showed that the MOSFET1. metal-oxide semiconductor field effect transistorVoltage-controlled field-effect transistor with an insulated gate, widely used in integrated circuits.2. metal-oxide-semiconductor field-effect transistorA common transistor type used here as the layout and technology reference. lot used in the design was sensitive to high-dose-rate radiation. Degradation appeared above 50 rad(Si)/s, even though the devices had been qualified for a total ionizing dose of up to 100 krad(Si). Exposure to high-dose-rate radiation reduced the threshold voltage by about 45 %.
The datasheet gives a VGSgate-source voltageGate-source voltage is the voltage between the gate and source terminals of a field-effect transistor.(th) range of 2.0 V to 4.0 V, so a 45 % reduction from a nominal 2.0 V threshold would bring the value to roughly 1.1 V. To evaluate the impact on circuit behavior, the threshold-voltage parameter was swept in PSpicepersonal simulation program with integrated circuit emphasisPSpice is a SPICE-based simulation tool for electronic circuits. simulations down to 0.5 V.
The simulations showed that the converter still operated normally, with the +5 V, +3.3 V, and -5 V rails remaining nominal even at the lowest threshold-voltage setting. The reason is that the MOSFET1. metal-oxide semiconductor field effect transistorVoltage-controlled field-effect transistor with an insulated gate, widely used in integrated circuits.2. metal-oxide-semiconductor field-effect transistorA common transistor type used here as the layout and technology reference.s are used as switching devices rather than in a linear operating mode, so the threshold-voltage shift did not prevent correct operation in this circuit. The same change would matter much more in a linear application.
The radiation-hardened counterpart identified for the MOSFET1. metal-oxide semiconductor field effect transistorVoltage-controlled field-effect transistor with an insulated gate, widely used in integrated circuits.2. metal-oxide-semiconductor field-effect transistorA common transistor type used here as the layout and technology reference. is JANSR2N7480U3. The reported analysis therefore links component sensitivity, radiation testing, and circuit-level simulation to a verified mitigation outcome for a space power supply.